欧美一区二区三区不卡视频 I 怡红院av一区二区三区 I 99热在线免费 I 激情综合色综合啪啪开心 I 衣服被扒开强摸双乳18禁网站 I 久久久久人妻一区精品下载 I 青草久久久 I aⅴ色国产欧美一本大道 I www.av在线.com I 91黄在线看 I 隔壁放荡人妻bd高清 I 丁香七月激情 I 色综合狠狠干 I 国产乱叫456 I 国产国拍精品av在线观看 I 中文字幕乱码熟妇五十中出 I 国产日本欧美在线 I 91视频在线观看大全 I 国产夜色av I 高h蛇全肉污文 I 亚洲精品不卡无码福利在线观看 I 亚洲国产精品无码久久久蜜芽 I 中国人做爰性生交视频 I www.欧洲在线观看 I 日本三级一区二区 I 色婷婷国产 I 久草视频污 I 日韩色影视 I 色综合偷拍 I 我们好看的2018视频在线观看 I 高潮内射免费看片 I a片免费视频在线观看 I 亚洲 综合 校园 欧美 制服

Welcome to the official website of TUNGSON ELECTRONIC MACHINERY LTD!
Collect this site | Return to homepage | Contact Us | Website Map |  Chinese
Popular searches on this site: AI automatic plugin machine Irregular plug-in machine Plug in machine manufacturer
Contact Us
TUNGSON ELECTRONIC MACHINERY LTD
Address: 5th Floor, Building B1, Songhu Zhigu Research Center, No. 6 Minfu Road, Liaobu Town, Dongguan City, Guangdong Province
Tel:0769-85389385
Fax:0769-85411416
E-mail:sales@tungson.hk
Are voids in SMT solder joints a problem?
Time:2024-12-01 18:12:35Source: Dongshun Automation Click: 210

The IPC Solder Product Value Association (SPVC) conducted a reliability study to determine whether the performance of various tin silver copper (SAC) alloys in lead-free alloys is equivalent in assembly, metallographic analysis and basic characteristics, thermal shock and temperature cycling. The conclusion of SPVC is that the performance of the three SAC alloys is not significantly different, and it is recommended to use SAC 305 as the preferred lead-free alloy in the electronics industry. Another result of this study is that when analyzing test boards using SAC lead-free solder paste, voids were detected. The cavity was marked on the test circuit board, but it was not repaired. In this case, the test circuit board was subjected to thermal shock and temperature cycling. The voids have also undergone thermal shock and temperature cycling, and SPVC also compares the voids in the solder joints.

The debate about solder joints

It is widely recognized in the electronics manufacturing industry that voids commonly seen in X-ray images may be a factor in classifying solder joints as non-conforming, especially when the size of the void exceeds 25% of the solder joint - especially when voids appear in BGA.

There has always been controversy in the electronic assembly industry regarding voids in solder joints. With the shift towards lead-free, controversy is becoming increasingly intense. The reason is that lead-free solder joints are more prone to forming voids than tin lead solder joints; Moreover, the percentage of voids in SAC alloy is higher than that in other lead-free alloys.

Test plan

Two types of lead-free circuit boards were used for testing in the IPC SPVC testing project: lead-free test board A * and lead-free test board B * *. The solder paste used for these two test boards is not specifically selected, but the same soldering flux is used. This way? Where is the beauty of Yan Mu? Private meal with hairy toes and sandpipers? Lai Mou Zhen Tian N Yi knocked and waved his surname, "Father of the Imperial Academy, how do you complain and fight? Apricot vomit??

In the lead-free test board A *, voids with an area exceeding 25% were observed on all circuit boards assembled using three types of SAC alloy solder paste, particularly on CSP84 lead-free components with a spacing of 0.5mm. The circuit board assembled with tin lead alloy clearly has voids, but on CSP84 components assembled with tin lead alloy with a spacing of 0.5mm, the void area is less than 25%.

On lead-free test board B * *, it was observed that the void area exceeded 25% on all circuit boards assembled with SAC alloy. On the circuit board, the voids in PBGA196, C-CSP224, and chip level package CSP8 all exceed 25%.

In order to determine the impact of voids on the reliability of solder joints, the testing scheme adopted by IPC SPVC includes the commonly recognized conventional temperature cycling and thermal shock in the entire industry. Environmental tests were conducted on both sets of test boards, and their functionality was monitored during the testing period. The test board includes circuit boards from two companies, each with four sets of forty boards. Three types of SAC solder alloy compositions and one low melting point (tin lead) solder are used for comparison. Each group took out a plate for destructive metallographic analysis, and this test plate did not participate in the temperature cycling study.

The temperature cycling scheme used reflects the IPC testing method. This temperature cycling scheme first maintains a low temperature (0 ℃) for ten minutes, then slowly rises the temperature to 100 ℃, and then maintains this high temperature for ten minutes before gradually returning to the low temperature state. The entire temperature cycle usually takes about 60 minutes. The cycle time is related to the time it takes for the furnace temperature to rise and the temperature stabilization process of the test board.

The thermal shock test plan is very similar to the one specified by JEDEC, which first maintains a low temperature (-55 ℃) for five minutes, then maintains a high temperature (125 ℃) for ten minutes, and then returns to the low temperature. The total cycle time is about 20 minutes. This cyclic process repeats continuously. Two sets of test samples were subjected to metallographic analysis after 500 temperature cycles per set.

test result

After environmental testing, this study compared the X-ray analysis results of the cavity, comparing the failure situation after 6000 temperature cycles, thermal shock, metallographic examination of both failed and normal solder joints, and comparing the results of metallographic examination. From these comparisons, and using several different statistical methods to compare temperature failure data and void location and size, we can clearly see that voids will not have any impact on the integrity of the solder joint.


After every 500 temperature cycles, remove the circuit board and perform penetrative X-ray imaging on each component on each circuit board. From this image, we can see that there are far more voids in SAC alloy solder joints than in tin lead alloy solder joints. In terms of quantity and size, CSP84 packaging solder joints have more voids than other array packaging solder joints. Comparing the cross-sectional images of packages that have undergone temperature cycling, we cannot see any clear correlation between voids and connection failure. For example, large voids can be seen in the cross-sectional view of the SAC 305 solder joints on test board A *, but this does not necessarily mean that these voids will cause connection failure - although this package has undergone 4500 temperature cycles.

On lead-free test board A *, for 84 input/output CPS packages with a spacing of 0.5mm, there are quite a few solder joint failures caused by creep fatigue caused by temperature cycling. From this, two parameters can be obtained, namely Weibull slope (β) and characteristic life (η) values. Figure 1 is a Weibull plot of the failure distribution of CSP84 packaging. The Weibull distribution indicates that the characteristic lifespan of SAC alloy solder joints is longer than that of tin lead solder joints (SAC alloy has 4713 to 6810 temperature cycles, while tin lead alloy has 1595 temperature cycles). However, on the circuit board without monitoring, the through X-ray images and cross-sectional views of every 500 temperature cycles indicate that there are significantly more and larger voids in the SAC alloy solder joints than in the SnPb solder joints. It is precisely because of this that each CSP84 package was inspected with X-rays after 6000 temperature cycles. We attempted to correlate the number of temperature cycles at which voids occurred with the occurrence of failure. Figure 2 shows Weibull values and η values. These statistical results were obtained from 24 CSP84 packages and 60 CSP84 packages. The 24 CSP84 packages were part of the IPC SPVC reliability test, while the 60 CSP84 packages were part of the reliability test for test board A. In an analysis, there were significant voids in the SAC387 solder joints assembled using conventional remelting techniques. However, there is no particularly significant difference in the characteristic lifespan of solder joints.

conclusion

We compared the number of voids and temperature cycles at which failure occurred in SAC connections based on the data provided by the IPC SPVC reliability research project on SAC alloys. We used eight independent statistical analysis methods (box plot, one-way ANOM, main rendering, matrix plot, etc.) to compare the number of cycles when a void exceeds 25% of the connection area and the number of temperature cycles when a void occurs. The comparison between the distribution of voids and the number of failure cycles indicates that voids do not affect the reliability of solder joints.

The number and size of voids in the solder joints were compared with the connection failure in temperature cycling data, and the conclusion is that there is no evidence to prove that voids in such SAC alloy solder joints will affect the reliability of the solder joints.


Prev14 principles of SMT zero defects  Next Next:What should be noted when selecting SMT surface mount machines?
Copyright ? 2025 TUNGSON ELECTRONIC MACHINERY LTD Technical support:Tuohai Network
13829276376
主站蜘蛛池模板: 中文在线а√在线 | 日本一区二区在线播放 | 亚洲精品中文字幕无码蜜桃 | 国产成人av一区二区三区在线观看 | 欧美激情一区二区三区 | 亚洲精品一本之道高清乱码 | 18禁黄网站男男禁片免费观看 | 久久综合久久综合九色 | 欧美人与动牲交a精品 | 日本免费一区二区三区最新 | 日韩激情无码av一区二区 | 国产精品白浆无码流出视频 | 久久99精品久久久久久秒播 | 性一交一乱一伦一色一情孩交 | 理论片87福利理论电影 | 无码人妻av一区二区三区波多野 | 久久精品国产99国产精偷 | 人人妻人人超人人 | 亚洲の无码国产の无码步美 | 456亚洲影院| 日韩v亚洲v欧美v精品综合 | 亚洲欧美不卡高清在线观看 | 精品无码久久久久久久动漫 | 一区二区三区日本久久九 | 国产在线aaa片一区二区99 | 免费人成视频在线观看网站 | 日韩一卡二卡 | 俄罗斯美女真人性做爰 | 无码无套少妇毛多18pxxxx | 丰满岳乱妇在线观看中字 | 人妻丰满熟妇无码区免费 | 亚洲女人的天堂www 少妇邻居内射在线 | 无码人妻精品一区二区蜜桃色欲 | 亚洲熟妇中文字幕五十中出 | 麻豆md0077饥渴少妇 | 日日摸天天爽天天爽视频 | 国产无遮挡又黄又爽不要vip网站 | 精品国产九九 | 亚洲欧美日韩国产成人精品影院 | 日本高清在线一区二区三区 | 中文字幕亚洲欧美日韩在线不卡 |